This is layer 2 or 3. It will be covered by the next few layers but I feel like it shouldn’t be this fugly. I’m using Cura’s Standard Quality except for temp which is set to 205. The filament is Inland PLA.

  • charmed_electron
    link
    fedilink
    English
    arrow-up
    9
    ·
    11 months ago

    Does that top surface feel ridged? To me this looks more like an issue with either overextrusion or z offset too low than temperature.

    • nomad@infosec.pub
      link
      fedilink
      English
      arrow-up
      4
      ·
      11 months ago

      I second z offset. Weird that this happens only at a certain regular “column”. Could be hiding an underextruded strand on the level below. In that case your temp might not be stable.

  • infinitevalence@discuss.online
    link
    fedilink
    English
    arrow-up
    6
    ·
    11 months ago

    i dont see an image?

    what type of Inland PLA, silk generally requires higher temps but some of the more standard ones print well at 180-190.

  • UniversalFlamingo@lemmy.worldOP
    link
    fedilink
    English
    arrow-up
    5
    ·
    11 months ago

    z offset / nozzle height seems to be the thing. I’ve raised it up and it looks better. After that I played with the temp a bit and it seems to be happier around 210-215 though there is more stringing.

    So far, all attempts at ironing have been a disaster, both zig zag and concentric. I’m going to continue dialing in the z offset and temp before ironing.

    • infinitevalence@discuss.online
      link
      fedilink
      English
      arrow-up
      1
      ·
      11 months ago

      Yeah, that looks much better. Do you have a self leveling bed? If your bed has a high point that is not captured in its measurements its possible that your still getting just a bit more drag in that specific spot.

      One thing you can do to test, is to move the print to a different spot on the bed in your slicer.

  • PatFusty@lemm.ee
    link
    fedilink
    English
    arrow-up
    2
    ·
    11 months ago

    To me it looks like your flow rate is too high. Calibrate your e-steps. That and raise your z offset. I don’t think it’s temperature related.

  • IMALlama@lemmy.world
    link
    fedilink
    English
    arrow-up
    2
    ·
    11 months ago

    I second running a temp tower. Your first layer may be a little too low, but you’re probably over extruding since it looks like your lower layers aren’t as wavy.

  • AliasVortex@lemmy.world
    link
    fedilink
    English
    arrow-up
    1
    ·
    11 months ago

    It’s primarily written for klipper, but I’ve been been getting pretty good results dialing in my was-an-ender with Ellis’ tuning guide (all but eliminated my problems with elephants foot). It goes over exactly what a good first layer should look and feel like, plus extra related settings.

  • UniversalFlamingo@lemmy.worldOP
    link
    fedilink
    English
    arrow-up
    1
    ·
    11 months ago

    Update: I wasn’t able to fiddle with it for a few days but after getting back to it have something I like.

    My current settings are based on the feedback in this thread and:

    z-offset made the single biggest difference. I reset the printer config and re-leveled.

    For this filament: https://www.amazon.com/Inland-1-75mm-White-Printer-Filament/dp/B084RDMG7C/

    Global Settings
    Layer Height		0.20
    Initial Layer H...	0.20
    Wall Thickness		0.80
    Top/Bottom T...		0.80
    Combing Mode		infill
    Build Plate Adh...	brim
    
    Extruder
    Wall Line Count		3
    Print Thin Walls	True
    Travel Speed		110
    Initial Layer Sp...	20
    Retraction Dist...	0.8
    Retraction Speed	45
    Minimum Extru...	1
    Brim Width		4
    
    Filament Print Settings:
    Default Printing Temperature	210
    Default Build Plate Temperature	 60
    Standby Temperature		195
    Fan Speed			100